I recently received a request to PWHT ALL Monel piping.
All the Monel piping is Schedule 10 and under 2".

Anyone know what might constitute a justification for this type of requirement?

Thanks in Advance

" There is no Shortcut to anyplace worth going "
 
Replies continue below

Recommended for you

Thanks metengr,
I reviewed the Bulletin and requested further information if available.

Thanks again

" There is no Shortcut to anyplace worth going "
 
In my opinion it's not necessary and usually not required a PWHT on a Monel material.

Solid solution alloys
Solid solution alloys are pure nickel, Ni-Cu alloys and the simpler Fe-Ni-Cr alloys. These alloys are readily fusion welded, normally in the annealed condition. As the heat affected zone (HAZ) does not harden, heat treatment is not usually required after welding

S.

Corrosion Protection & Corrosion Control
 
Which alloy? 400?
What sort of PWHT are they asking for?

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
B-165 , 400

" There is no Shortcut to anyplace worth going "
 
Just for the record, I wanted to let you folks know that
(since I asked the question, I learned) Welded MONEL alloy 400 components normally go into service as welded.(that part I knew) If there is a concern that the enviironment could induce stress corrosion cracking (e.g, steam containing ammonia), the structure could be stress relieved by heat treatment at 1150 to 1400 deg.F. We have the potential for these trace elements and are looking to increase the odds of a successful installation.