Do you need to PWHT fillet welds in A333 gr6 pipe
for propane duty down to -43degC ?
 
Replies continue below

Recommended for you

To answer your question, what Code or Piping Standard are you working under - ASME B31.3 or B31.4 Process Piping Standard or other? Also, what is the pipe size/schedule?

Second question - are you sure about fillet welds or are these butt welds with external fillets applied like a branch connection or combination or are you welding attachments to existing piping? Please be specific.


 
Why are you using fillet welds on Propane duty? Butt welds are a much safer proposition.
 
We are working to B31.3, pipe is 3/4" sch. 80 and the reason we are using socket weld fittings is because that is the existing site standard.
 
No PWHT. I checked B31.3, Table 331.1.1, for 3/4" wall thickness and less for P-No 1 base material, no PWHT.
 
metengr.
I know B31.3 says no PWHT for P 1 materials but, do environmental conditions change the requirement for PWHT even though is not mandatory.
 
No. ASTM A 333 Grade 6 is basically a medium carbon steel with 0.2-0.3% Mo. This is a weldable grade of steel, considering Section IX treats it like a P-No1, Group - No1 material. For your application, this material should pose no problems without PWHT.
 
Paulbrown,
metengr answers your question explicitly. It's what I advised Reg anyway!!!
 
Thanks Metengr.

DSB123 - We don't usually get to know whether questions have been asked or answers given !!!
 
Paulbrown,
As metengr has stated, B31.3 does not require PWHT for the low temperature service. Furthermiore, it is not common practice to PWHT with the design described; however, service conditions, as determined by the designer, may dictate otherwise. "In such cases, the designer may specify more stringent requirements in the engineering design, including heat treatment.." (ref. 331.2.2)

 