I need to x-ray & /or Ultrasonic test some parts made from Carburized AISI 9310 steel, 3 of 5 parts had heat treat cracks.
I need to verify the two parts do not have cracks below sub-surface. any recommendations?

parts past mag particle insp,but I want to make sure there are no defects at the center.

Thanks
Mfgenggear
 
Unless your parts are thicker than about 2-inches, or have a convoluted geometry, Wet Fluorescent Fully-rectified DC mag-particle will find your subsurface problems. The MT is what you will get in a 'bench MT booth'. Not really possible to duplicate it 'in the field'.

Otherwise, have them UT scanned using 70-degree and 45-degree transducers "Client info -- No Cracks"
 
Duwe6

I not sure I under stand your statement

Yes the MPI was done with an fully rectified Mag. Isso Approved.

My understanding is Mag will detect surface defects same as
penetrant. X-ray & ultrasonic will detect sub surface defects. I am a levell II except I have not been in practice for xx number of years.

no X-ray? why please advise.

Mfgenggear
 
mfgenggear

If the 3 parts were rejected due to surface-breaking heat treat cracks, why should you suspect the other 2 parts(already succesfully passed the MPI) have sub-surface cracks i.e. not heat treatment.

As your sector is aerospace I would guess part geometry may be complex and to PROVRE no sub-surface cracks present you will need to perform extensive NDT, both UT and RT as you have no idea of defect location. An odd random X-ray or a few UT scans will not guarantee freedom from haphazardly oriented cracks. That is process quality control's responsibility.

Talk to your Level III or approach Level III consultants.
 
NDEguy

we have a level 3 only in mag & temper etch,
we normally send out all x-ray or UT to an out side source.
hence I need a spec that details the actual procedure.
I no longer due NDT I am now an Mfg Engineer.

any suggestions

Mfgenggear

 
So if you send the 2 parts out to your local RT/UT shop with the instruction find all sub-surface cracks without limitations on size, position or orientation, you will be offering them a blank check! And as for a guarantee you will only ever be relying on what your NDT shop determines as sufficiently comprehensive examination.

If failure analysis of the 3 cracked parts reveals the reason for the failure then you can perhaps understand why the other 2 parts did not fail and if there is any reason to suspect the internal quality of the material.

I dont feel this helps you much because its the old NDT bind - how much work and money is justifiable for the desired end result of a "No significant defect" report. Basically, what are the parts worth to you?
 
NDE Guy

I understand

There is a in-process failure analysis for the corrective action from our Heat Treating Vendor.
To my experience it is very rare for 9310 steel to crack.

But I have two possible good parts that where acceptable to MPI. and that is all I am required by contract (ASTM E1444)&
Mil-Std-1907 Grade A except no Indications permitted.

base on that criteria could I apply it to X-ray ?
is there an equivlant ?

Thanks
Mfgenggear

 
mfgenggear: DC MT will reveal subsurface defects. There is a limit to the size of defect detectable, depending on how deep that defect is. Google "Ketos Ring". You may be thinking of AC MT. The AC magnetic field makes it a "skin effect" and will only detect defects open to the surface.

As to "no x-ray / RT": crack orientation is very critical for detectability, and each RT costs money. Taking RT 'shots' every few degrees in a full 360-deg circle will be VERY costly. UT scanning is MUCH faster, thus much cheaper. Additionally, it is MUCH easier to find tight cracks using UT versus RT.
 
Duwe6

Very well thanks

Mfgenggear
 