Hi there
I require chromium and carbon's diffusion coefficient in ferritic stainless steel.
Any references?
Thanx :)
 
All I could find right now is the variation of diffusion coef. w/ temp. for Carbon in bcc-Fe.

D=2x10^-6 exp(-84300/RT)

Units m^2/s

Nick
 
From “Diffusion Data of various Element in the Matrix with Iron or Iron Alloys,” data from Technology Reports of the Tohoku University, vol.47~48,
you can find diffusion data for Cr in Fe & Fe-Cr alloys at
and diffusion data for C in Fe and a number of Fe alloys at

Note: the data are presented in tabular form such that you can select which data to use, then enter the temperature (oK) at the bottom, and the diffusion coefficient will be calculated for you. Log D vs. 1/T can also be plotted. The closest alloy listed is Fe-13%Cr for which D = 3.32 x 10-16 m2/s at 1073K.

Note: there doesn’t seem to be much diffusion data for C in Fe-Cr alloys, but it appears that the diffusion rate for C in Cr-1%Fe is about 10% that for C in bcc-Fe, so it would be reasonable to reduce the diffusion coefficient for Fe-12%Cr by about 1% from that for bcc-Fe.

You might also be interested in another on-line resource:
“Review on Lattice Diffusion of Substitutional Impurities in Iron. A Summary Report”
Hiroshi OIKAWA ( 1982)
For diffusion coefficient of Cr in bcc-Fe at 1048-1971K, Do = 2.33 x 10-4 m2/s, Ea = 238.8 KJ/mole.
 