Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations The Obturator on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Mixing SS alloys in a dam saltwater environment

Status
Not open for further replies.

RoyHobart

Marine/Ocean
Aug 14, 2010
2
Any problem having different SS alloys in contact in a damp saltwater environment? Specifically, I'd like to put a 316 collar on a 431 propshaft - but I won't do so if the different alloys could lead to galvanic corrosion.
 
Replies continue below

Recommended for you

The title of the thread is slightly misleading - I meant to say 'Damp' rather than "dam" :)
 
You will may get serious corrosion of the 431.
I would suggest that you use a non-ferrous alloy.
Maybe a CuNi.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
In my opinion the problem is not the galvanic corrosion, that should be negligible between two stainless steel(see FAQ at page 22 of the doc below)



The problem that i see is the corrosion resistance of the 431 in contact with seawater. it has approx the same resistnace of SS 304.

"Reasonable resistance to salt water in cold southern waters but less resistant than Grade 316 in tropical waters. Overall the corrosion resistance of 431 is approximately the same as or slightly below that of grade 304.
"