Dear colleagues,

Could you give me any advice about evaluation of microstructure of steel 38MnVS6.

Only ferritic-perlitic structure is acceptable.

If sample 2 microstructure consists from ferrite and perlite (+sorbite?) microstructure of sample 1 consists from ferrite, perlite, bainite (lower?) and martensite. It is my opinion, but I have very small experience in microstructure of this steel...

Please let me know your opinion.

Thank you in advance
 
 http://files.engineering.com/getfile.aspx?folder=d016d281-6d76-49ba-a4f3-dadf0a28e0ff&file=Sample1.jpg
Your sample #2 microstructure looks like a dual-phase steel consisting of ferrite and fine and coarse pearlite. Your sample #1 has other transformation products besides ferrite and pearlite, and is not a dual-phase steel.
 
I agree with metenger.
The company I work for makes this grade on a fairly regular basis, and sample 1 does appear to have bainite. I wouldn't commit to martensite from a black and white micro-photo, but the wider streaks all running in one direction look suspiciously like it. Especially if they appear gold-ish after a picral etch, which this appears to be.

Out of curiosity, what is the application? I know 38MnVS6 is typically for bolts and the chem is designed so that there is no 'need' for heat-treating after rolling...

"Metal Health'll cure your crazy
Metal Health'll cure your mad
Metal Health is what we all need
It's what you have to have"

-Quiet Riot
Bang Your Head (Metal Health)
 
Status
Not open for further replies.

Part and Inventory Search

Sponsor

Back
Top