Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations TugboatEng on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Length of pipe to be used in PQR 1

Status
Not open for further replies.

AliGrailly

Mechanical
Joined
Dec 8, 2020
Messages
72
Location
IR

Hi

We prepared a welding piece for pqr flange A350-LF2 to pipe A333-6 Thk 8mm filler Er80sni1 , in UG-84 not mentioned the length of pipe to be cut for sending to lab
350mm is enough???

 
Look in Section IX for answer - not Section VIII.
 

Refer to code ix ... 10x10 but thk is 8 mm
 
AliGrailly
You are very confused. Consult a welding engineer.

Regards
 
Dear Ali,[wavey]
salam

Kindly find below notes:

1-length and number of test coupon shall consider in PQR preparation.

2-At the first you shall refer to project specification. if there is note any note in spec refer to related welding code./standard such as AWS D1.1/ASME IX ,ISO 15614.

3-ASME IX has not define special length for pipe test coupon. According to QW-210 : "The dimensions of the test coupon shall be sufficient to provide the required test specimens." length of pipe test coupon shall be sufficient to obtain the longest specimens such as tensile and bend.

4-25cm is good for length of pipe test coupon. if you face shortage material may reduce length but it shall be consider that if length of test coupon is very short its affect on Interpass temperature and cooling rate and affect on hardness and impact test result.

5- if external or internal clamp used for fit-up, length of clamp shall be consider.
6- for such diameter such as 32",42",etc its prefer to cut 50cm test coupon.