How to decide the corrosion allowance while designing a vessel

Status
Not open for further replies.

grnblr

Electrical
Joined
May 1, 2002
Messages
14
Location
IN
Could anyone tell me how to select the corrosion allowance required to be assumed while designing a vessel, in particular for a high pressure ammonia storage receiver used in a refrigeration plant.

Pl help. Thanks in advance

grnblr
 
The typical anhydrous ammonia storage tanks are constructed of stress relieved, carbon steel in accordance with ASME Section VIII, Div 1 requirements. From my experience with our power plant SCR's that use ammonia injection, our design specification for ammonia storage tanks required a 1/8" corrosion allowance. The 1/8" is a common value used in pressure vessel design. I would see no difference for your application. Remember, the corrosion allowance is not taken credit for in calculating minimum vessel wall thickness.
 
Corrosion allowances are determined from established corrosion rates of a material exposed to a corrosive media, concentration and temperature of exposure and then deciding the desired service life of the vessel. There are a number of resource books available to provide corrosion rates.

 
You must determine the amount of moisture in the ammonia. A little moisture will greatly reduce the corrosion rate.
 
Metalguy;
The moisture content can vary from 0.2 to as much as 0.5 percent, but must remain above a minimum threshold of 0.2 percent by weight to prevent SCC of carbon steel by liquid ammonia with any entrapped air in the vessel.
 
Thanks metengr

the details will help