Arthur,
I have reviewed every ASTM standard related to steel forgings, but cannot find anything on decarburization limits. ASTM A837 Standard Specification for Steel Forgings, Alloy, for Carburizing Applications shows grade 8620, but there is no mention of decarburization or limits. ASTM A788 Standard Specification for Steel Forgings, General Requirements is the general spec for steel forgings, and there is no mention of decarb here either. Two other forging specs for gear applications, A290 and A291, similarly do not reference decarburization limits. The only one I could find that even mentions decarb is A579 Standard Specification for Superstrength Alloy Steel Forgings, but only as a Supplemental requirement, and even then the purchaser still has to specify the limits. Perhaps you are thinking of an SAE AMS or other standard.