jerin james
Mechanical
Hello Sirs,
We have got below feedback from a Reputed Cladding mill regarding Inconel 825 being subject to PWHT. You might wonder why PWHT is required for Inconel 825, the base material is CS , Inconel 825 is the cladding material .
quote
The PWHT is limited through sensitization. A PWHT of 630°C for the requested holding time (up to 9h) would be ok for the base material but the corrosion resistance properties of the clad material would be strongly deteriorated. In case the PWHT will be carried out at 630° & holding time up to 9h, there is no chance to meet the corrosion resistance requirements as per ASTM G-28 practice A.
Acceptance criteria of 0,457mm/y could be confirmed for a PWHT of 575°C for 9 hours in total when using alloy 825 as cladding material. In figure below the max. possible PWHT is pictured:
Unquote
Above reference from Fig 1 of ASTM G-28 (check attached) is theoretical we understand.
However, another Reputed mill has confirmed to guarantee corrosion resistance after PWHT , we are actually confused.
Experts can we have your advise.
Thanks
We have got below feedback from a Reputed Cladding mill regarding Inconel 825 being subject to PWHT. You might wonder why PWHT is required for Inconel 825, the base material is CS , Inconel 825 is the cladding material .
quote
The PWHT is limited through sensitization. A PWHT of 630°C for the requested holding time (up to 9h) would be ok for the base material but the corrosion resistance properties of the clad material would be strongly deteriorated. In case the PWHT will be carried out at 630° & holding time up to 9h, there is no chance to meet the corrosion resistance requirements as per ASTM G-28 practice A.
Acceptance criteria of 0,457mm/y could be confirmed for a PWHT of 575°C for 9 hours in total when using alloy 825 as cladding material. In figure below the max. possible PWHT is pictured:
Unquote
Above reference from Fig 1 of ASTM G-28 (check attached) is theoretical we understand.
However, another Reputed mill has confirmed to guarantee corrosion resistance after PWHT , we are actually confused.
Experts can we have your advise.
Thanks