I have a WPQR for GMAW overlay welding, filler mat AWS/ASME SFA - 5.21 ERCCoCr-A and base material WCB. and I have welder qualifications of this WPQR. However, customer needs filler material to be AWS/ASME SFA - 5.21 ERCCoCr-E.
If every essetial variables are same and only change is the filler material, do I need a new WPQR and welder qualifications for new filler material.
F-no of the filler material's are same (72) acc. to Table QW-432 (ASME BPVC.IX 2023). SFA no is same.
Base material and all other parameters will be the same on WPSes.
Additionally, totally different question, if I do this overlay weld by non-stop automatic welding on a circular pattern, does it count as 1 run, or does every complete turn counts as +1 run. So, for the seat welding of a valve, If I am welding the seat surface on 3 turns, weld height increases on every turn, does it count as 3 runs or 1 run?
If every essetial variables are same and only change is the filler material, do I need a new WPQR and welder qualifications for new filler material.
F-no of the filler material's are same (72) acc. to Table QW-432 (ASME BPVC.IX 2023). SFA no is same.
Base material and all other parameters will be the same on WPSes.
Additionally, totally different question, if I do this overlay weld by non-stop automatic welding on a circular pattern, does it count as 1 run, or does every complete turn counts as +1 run. So, for the seat welding of a valve, If I am welding the seat surface on 3 turns, weld height increases on every turn, does it count as 3 runs or 1 run?