Nov 13, 2005 #1 bmoorthy Mechanical Joined May 29, 2003 Messages 457 Location CA Hello all What does the number ASTM Grain size 0, 1, 2 signify? Does it signify number of grain boundraies the examiner can see in a given unit length (Say Micron)?
Hello all What does the number ASTM Grain size 0, 1, 2 signify? Does it signify number of grain boundraies the examiner can see in a given unit length (Say Micron)?
Nov 13, 2005 1 #2 Goahead Aerospace Joined Jul 13, 2003 Messages 625 Location IL The ASTM Grain Size Number N is defined by ASTM E-112 as N = (log n/log 2)+ 1.0000 where n is the number of grains per square inch at 100x It used to be compared visually with published charts, but modern software is available that can calculate and return ASTM Grain Size Number. Regards, http://www.welding-advisers.com/ Upvote 0 Downvote
The ASTM Grain Size Number N is defined by ASTM E-112 as N = (log n/log 2)+ 1.0000 where n is the number of grains per square inch at 100x It used to be compared visually with published charts, but modern software is available that can calculate and return ASTM Grain Size Number. Regards, http://www.welding-advisers.com/
Nov 13, 2005 #3 metengr Materials Joined Oct 2, 2003 Messages 15,478 Location US As gohead mentioned, the ASTM grain size scale was established by ASTM to provide a quantitative comparison of grain size for metals and alloys. The higher the ASTM grain size number, the finer or smaller the grain size. Upvote 0 Downvote
As gohead mentioned, the ASTM grain size scale was established by ASTM to provide a quantitative comparison of grain size for metals and alloys. The higher the ASTM grain size number, the finer or smaller the grain size.
Nov 15, 2005 #4 SJones Petroleum Joined Apr 22, 2001 Messages 3,948 Location GB Why not get the standard and become familiar with the requirements? Steve Jones Materials & Corrosion Engineer http://www.pdo.co.om/pdo/ Upvote 0 Downvote
Why not get the standard and become familiar with the requirements? Steve Jones Materials & Corrosion Engineer http://www.pdo.co.om/pdo/