glass fails in tension so you should look for the maximum stress intensity
actual failure levels quite strongly dependent upon surface finish/or roughness, polished surfaces are best and failures generally initiates at the edges
typical values would be 2000 psi for tension but upwards of 40,000 psi in compression
schott has data relating to rate-of-stress application vs failure
Weibull analysis generally used for this kind of failure
be very cautious about the restraints/boundary conditions for any material that is subject to brittle failure
look for works by P Yoder and V Genberg