1) The best etchant formula to reveal the weld penetration of 304 stainless steel ?
2) After etching, will the HAZ show up too which confuses the reading for penetration ?
3) The underlining etching mechanics?
thanks.
 
1. Without more details, this is not an easy question. Electroetching with 10 % oxalic acid, Kalling's, Beraha's, Ralph's, and others are all possibilities.
2. Weld metal/fusion zone should be distinct from HAZ after etching.
3. Different mechanisms are present for different etchants. Anodic dissolution of grain boundaries, sulfide film formation, and others are present.
 
Thanks metengr!

Best regards - Al
 
Carbides will only be present if you have high enough carbon and the cooling rate is slow enough.
A light electrolytic etch in 10% oxalic acid will work well, don't over etch.
Most etchants rely on differential attack rates for various phases/orientation/compositions.

= = = = = = = = = = = = = = = = = = = =