Hello.

I have a problem with modelling of ECAP (Equal Channel Angular Pressing) process. The problem is, that the mesh distorts heavily – it looks like the material (billet) flows between the punch and the die during the processing:
2025_07_05-11_14_06.png

The assembly is given below:

2025_07_05-10_43_50.png

The ECAP canal has 10 x 10 mm rectangular dimensions.

I am using:
  • Punch and die are discrete rigid parts
  • Abaqus Explicit with 0.2 s time step.
  • Z symmetry
  • 0.1 friction coefficient (but tried also higher)
  • I tried general contact and surface-to-surface contact
  • I made tie between the punch and billet – this helped a little – nodes on the top surface of the billet didn’t move relative to the billet, but billet’s nodes below them moved
Screenshots with details are given below:

2025_07_05-11_18_46.png


Young's modulus is 44700.
Poisson's ratio is 0.35.
Density equals 1.75e-9.


2025_07_05-11_20_38.png


2025_07_05-10_50_50.png
2025_07_05-10_51_45.png
2025_07_05-10_51_49.png

2025_07_05-10_56_15.png

2025_07_05-10_57_34.png

I am attaching also .inp file.

What am I doing wrong?
 

Attachments

Solution
Make sure that the proper side of the punch bottom surface is selected. Try adding some point mass/inertia to the rigid body reference point. You should also consider replacing discrete rigid bodies with analytical rigid surfaces whenever possible. Check the energy outputs (especially ALLKE and ALLAE vs ALLIE).
Make sure that the proper side of the punch bottom surface is selected. Try adding some point mass/inertia to the rigid body reference point. You should also consider replacing discrete rigid bodies with analytical rigid surfaces whenever possible. Check the energy outputs (especially ALLKE and ALLAE vs ALLIE).
 
Solution
It works. Thanks FEA way.
What helped was to replace the discrete rigid punch with the analytical rigid punch.
Second thing, which was necessary is the use of surface-to-surface contact. Using the general contact generates errors.

The next step is to add heat analysis to it. The problem is, that analytical rigid parts do not exchange heat.
 
It works. Thanks FEA way.
What helped was to replace the discrete rigid punch with the analytical rigid punch.
Second thing, which was necessary is the use of surface-to-surface contact. Using the general contact generates errors.

The next step is to add heat analysis to it. The problem is, that analytical rigid parts do not exchange heat.
Update:
It works also with discrete rigid punch, but surface-to-surface contact must be defined also for sides of the tools. Previously I defined contact surface only for bottom surface of the punch.
 
I have a new problem. I am getting very high strains in a billet, where it is in contact with the die. It should not be like this. What may be the cause?