Hello,

I have some carbon steel straps
(length=10" xsection: .06"x1.25")
that see some friction and some humidity (indoor environment).

Ideally, I'd like a wonder paint that is very tough, completely
rustproof and can't be scraped off, but that all seems mutually
exclusive. I could even see period application of furniture wax or
similar working.

Are there any FAQs or references people can cite, so I can review the
available approaches and technologies ?

Thank you,

 
You could coat the parts with Teflon.


Tunalover
 
PowderCoatings are very tough and durable. They all have pinholes though.
 
You want reliable abrasion resistance and corrosion resistance in a polymeric coating? Epoxy powdercoat. You want just abrasion and corrosion resistance? Hot-dip galvanize. If it's indoors though, you may get away with merely a heavy zinc electroplate coating.
 
how much cost can you afford?
 
I have been reviewing my original question and the
very thoughtful recommendations.

I went to the local hardware store today, and the shopkeeper
suggested Car Wax and/or boiled linseed oil.

I mentioned it was for indoor use, but I think I'm after a "farmer's almanac" approach that people would use on their favorite handsaw- As long as it's not oily and

1) it's cheap
2) it's ok if it's periodically reapplied

thanks again for all the replies.

 