Inadequate PWHT holding time for Carbon Steel piping in caustic service (NACE SP-0403)

Status
Not open for further replies.

kondori

Materials
Joined
Feb 3, 2012
Messages
7
Location
DE
Dear all,

We have a situation in our project (petrochemical plant construction) where in our caustic service piping (mostly 4-6mm wall thickness and small OD), all the weldments have been post-weld heat-treated, but it has been done acc. to ASME B31.3 (not as per NACE SP-0403 requirements). The PWHT holding temperature has been around 600- 620C, and the holding time is 30 minutes in almost all cases. As you know, NACE SP-0403 asks for a minimum holding time of one hour and a temperature range of 635+_14 C.

At this stage of the work, going back and repeating PWHT ACC. to NACE SP-0403 will be a nightmare. Considering the ASME PWHT has been done, we believe that these weldments still have a chance and should not be rejected without further evaluation, and that's why I am posting this thread.

What is the correct way forward here...?
I presume we have to cut a sample (or samples) of a welded joint (or prepare a PQR test coupon) and send it for corrosion testing. I can go through the available references myself and find something, but I do not pretend to be a corrosion engineer, and I do not want to make mistakes here.
Please note that all the field hardness test results have been satisfactory.

Thank you for your time and assistance.
 
Last edited:
In B31.3 2022 Table 331.1.1 the holding time is 15 min min. for P-1 material.
 
In B31.3 2022 Table 331.1.1 the holding time is 15 min min. for P-1 material.
Our PWHT meets the requirements of ASME B31.3.
That's not the issue.
The issue is that we did not meet the NACE SP-0403 requirements.
 
Should I tell you how many thousands of hardness reading it would take make me feel any comfort about this.
How are you checking hardness on the ID of the welds and HAZ?
Look at your actual chemistries, where are they in terms of CE?
Look at the actual data from the PWHT.
Were the times and temps to the low side or the high side?
If the CE is low and the the times and temps are high then you are not off by much and this might work.
Is re-PWHT more of a nightmare than in service failures?
Are you ready to put it into the record that you signed off on these deviations?
 
Should I tell you how many thousands of hardness reading it would take make me feel any comfort about this.
How are you checking hardness on the ID of the welds and HAZ?
Look at your actual chemistries, where are they in terms of CE?
Look at the actual data from the PWHT.
Were the times and temps to the low side or the high side?
If the CE is low and the the times and temps are high then you are not off by much and this might work.
Is re-PWHT more of a nightmare than in service failures?
Are you ready to put it into the record that you signed off on these deviations?
Thank you, EdStainless, for your reply.

Update:
Today, I found out that originally, they have been following the specification and performing PWHT acc. to NACE SP-0403. The reason why they have changed things and reduced the holding time & temperature has been due to excess distortion and oxidation after PWHT. The EPC contractor has submitted a TQ, to reduce the holding time to 30 minutes (as a solution), and they have received approval for it (this has fixed the excessive distortion & oxidation issue, though).

Answers to your questions:
- The field hardness tests have been obtained only from testing the outside surfaces (due to lack of access to the inside of our small-OD caustic piping system), but we did lab hardness tests from inside during qualification tests (PQR), and they were mostly around 120 HV (never above 140 HV).
- Our material is NACE MR0175 certified, and the CE numbers are low.
- We have always had good control over our PWHT operations, and we repeat the PWHT anytime we detect any deviations in time/temp parameters. Please note that our PWHT holding temperature has been around 600- 620C, and the holding time is 30 minutes in almost all cases.

Considering the above information and the fact that residual stress levels should be considerably lower after PWHT, I also do not think this piping system would cause huge problems in operation. Yet, I am looking for a way (especially corrosion testing) to make sure that's the case. I would rather have some favourable corrosion test results to rely on when signing off on such deviations.

Thank you again,
 
Last edited:
your customers standards for their process govern.
 
1) If preheat was performed before welding, I can tell you that for 4mm to 6mm wall thickness (small pipe diameter), 30 minutes PWHT is adequate. 2) Also refer to Figure 1 in NACE SP-0403 "carbon steel no stress relief necessary"
 
If you go for various lab tests like metallography, hardness, tensile strength etc., you won't get much difference between samples heat treated as per NACE or ASME.
I have faced such situation and the non-conformity that I raised was closed based on such tests.
I was a quality assurance / control engineer at that time and the project manager could not understand the real consequence of such poor fabrication practice as a service failure might take place say after 5 years of commissioning and no failure analysis would detect the real cause of failure which would be poor fabrication / quality control practice at the project stage.
But the pertinent question here is who you are and what sort of organization are you working for.
 
More
1) Did you perform hardness tests before and after PWHT?
2) Did you control the heating and cooling rate during PWHT?
 
Who signed off the TQ approving the reduction in time ?
Our role in Quality is to identify issues and communicate these to the relevant engineers.
It is the Engineering department who ultimately decide if the request is acceptable.
IMHO this should not have been a TQ but a Deviation and therefore Client sign off is imperative.
 
Does your caustic concentration and metal temperature show the welds to be in Area A, B or C of Figure 1 of NACE SP-0403 ?
As stated - Engineering are responsible for providing this information, not Quality.
 
Thank you all for your replies.

For clarification, this is where we are at the moment:
  1. We are the owner of the plant (Quality Dep.)
  2. Caustic concentration and metal temperature show the welds to be in Area B of Figure 1 of NACE SP-0403.
  3. Additionally, our specification requires PWHT at 630C for a minimum of 1 hour of holding time for all the welds in caustic service.
  4. Originally, the EPC contractor had been following the specification and performing PWHT acc. to NACE SP-0403 (1 hr at 630C), but they faced excessive distortion and oxidation (after PWHT) in these small-diameter piping installations. Instead of introducing measures to control oxidation and distortion, the EPC contractor has submitted a TQ to reduce the holding time to 30 minutes and the holding temperature down to 600- 620C as a solution, and they received approval for it (this has fixed the excessive distortion & oxidation issue).
  5. The EPC contractor has already completed the installation. We found out about this issue when we were reviewing the QC reports (after the installation of caustic piping was completed). We asked for their justification for this change, and they submitted their approved TQ. Our further investigation revealed that they have done this only to prevent excess distortion and oxidation after PWHT in these small-diameter piping installations (with no consideration of corrosion performance).

At this point, all I can think of (as to how to proceed with this NCR) is to cut out samples (or prepare new test coupons) and send them for laboratory (corrosion) tests and make a decision based on those results. Otherwise, we would have to either leave it as it is or reject the whole installation, and I do not like either of these options. That is the main reason why I have posted this thread. Has anyone ever done anything like this...? If so, I would be grateful if you could provide me with some detailed information (e.g. type of tests, acceptance criteria, etc.)

Thank you again.
 
Last edited:
I guess there are 2 issues here, 1) Contract acceptance 2) Plant performance., but I'll preface this with a few points

A) From my experience with CSCC -> It's not an exact science, the NACE curves should be considered guidelines with quite wide bands. Depending on the fluid and other impurities the exact point of CSCC happening can be vastly different from the curves. I have no idea where your particular service falls, and also have no idea what controls are in place to ensure the fluid stays within design limits (in particular ensuring temperature limits are not exceeded)
B) CSCC tends to be a slower / long term issue, unless there is some real obvious temperature excursion in operation, so given your situation the difference between "proper" heat treatment and not is likely not to show up for a long time (I'd suggest years to decades), even if at all.
C) As per Dhurjati Sen above, lab testing is unlikely to give a pass / fail in any meaningful way
D) As a plant operator / owner, regardless of any of the above, I would always put some sort of inspection program in place to look for signs of CSCC, this would typically be in the form of periodic MPI inspections on the internal of pipes and vessels -> there is a whole world of in's and outs of detecting CSCC

So back to the start
1) Contract acceptance -> have fun with that, but your likely outcome is some compromise and acceptance discount or something, noting this is an issue that senior management should deal with, not an engineer

2) Plant performance -> I'd suggest that if the situation was accepted as is, all that could be said is that "there is an increased likelihood of CSCC occuring" This then becomes a question of risk, it's not black and white (however noting even when PWHT is done properly, you can still have CSCC failures). I'd suggest a mitigation would be to implement more onerous testing for the presence of CSCC, this would likely look like yearly MPI of a sample on internal pipe welds, randomly selected in the various pipelines of concern. This would be intrusive, but ultimately is the trade off that is likely required. This is generally the world I live in, developing practical inspections / maintenance / whole of life strategies for operating plants.

In summary
Option 1) Leave as is and do nothing (cheapest, not a good idea)
Option 2) Get everything re PWHT (has a cost, may or may not be higher than option 3)
Option 3) Accept CSCC is more likely to occur, and implement a more onerous inspection program / try to cost the risk of potential failures and future pipeline replacements (has a cost, compare to option 2)
 
Be practical. Use the pipes as they are and increase in-service inspections..
 
I guess there are 2 issues here, 1) Contract acceptance 2) Plant performance., but I'll preface this with a few points

A) From my experience with CSCC -> It's not an exact science, the NACE curves should be considered guidelines with quite wide bands. Depending on the fluid and other impurities the exact point of CSCC happening can be vastly different from the curves. I have no idea where your particular service falls, and also have no idea what controls are in place to ensure the fluid stays within design limits (in particular ensuring temperature limits are not exceeded)
B) CSCC tends to be a slower / long term issue, unless there is some real obvious temperature excursion in operation, so given your situation the difference between "proper" heat treatment and not is likely not to show up for a long time (I'd suggest years to decades), even if at all.
C) As per Dhurjati Sen above, lab testing is unlikely to give a pass / fail in any meaningful way
D) As a plant operator / owner, regardless of any of the above, I would always put some sort of inspection program in place to look for signs of CSCC, this would typically be in the form of periodic MPI inspections on the internal of pipes and vessels -> there is a whole world of in's and outs of detecting CSCC

So back to the start
1) Contract acceptance -> have fun with that, but your likely outcome is some compromise and acceptance discount or something, noting this is an issue that senior management should deal with, not an engineer

2) Plant performance -> I'd suggest that if the situation was accepted as is, all that could be said is that "there is an increased likelihood of CSCC occuring" This then becomes a question of risk, it's not black and white (however noting even when PWHT is done properly, you can still have CSCC failures). I'd suggest a mitigation would be to implement more onerous testing for the presence of CSCC, this would likely look like yearly MPI of a sample on internal pipe welds, randomly selected in the various pipelines of concern. This would be intrusive, but ultimately is the trade off that is likely required. This is generally the world I live in, developing practical inspections / maintenance / whole of life strategies for operating plants.

In summary
Option 1) Leave as is and do nothing (cheapest, not a good idea)
Option 2) Get everything re PWHT (has a cost, may or may not be higher than option 3)
Option 3) Accept CSCC is more likely to occur, and implement a more onerous inspection program / try to cost the risk of potential failures and future pipeline replacements (has a cost, compare to option 2)
Thank you, Andrew.
Option No. 3 seems to be the most reasonable solution.
I will propose options 2 & 3 to the project management (so they choose option No.3).
 
Dear all,

We have a situation in our project (petrochemical plant construction) where in our caustic service piping (mostly 4-6mm wall thickness and small OD), all the weldments have been post-weld heat-treated, but it has been done acc. to ASME B31.3 (not as per NACE SP-0403 requirements). The PWHT holding temperature has been around 600- 620C, and the holding time is 30 minutes in almost all cases. As you know, NACE SP-0403 asks for a minimum holding time of one hour and a temperature range of 635+_14 C.

At this stage of the work, going back and repeating PWHT ACC. to NACE SP-0403 will be a nightmare. Considering the ASME PWHT has been done, we believe that these weldments still have a chance and should not be rejected without further evaluation, and that's why I am posting this thread.

What is the correct way forward here...?
I presume we have to cut a sample (or samples) of a welded joint (or prepare a PQR test coupon) and send it for corrosion testing. I can go through the available references myself and find something, but I do not pretend to be a corrosion engineer, and I do not want to make mistakes here.
Please note that all the field hardness test results have been satisfactory.

Thank you for your time and assistance.
API 571 reads:

Cracking can be effectively prevented by means of a stress-relieving heat treatment (e.g. PWHT). A heat
treatment at 1150 °F (620 °C) minimum with a minimum holding time of 1 hr is considered an effective stress
relieving heat treatment for carbon steel.

What will be the operating temperature of the system? That would determine my level of concern with the holding time.
 
API 571 reads:

Cracking can be effectively prevented by means of a stress-relieving heat treatment (e.g. PWHT). A heat
treatment at 1150 °F (620 °C) minimum with a minimum holding time of 1 hr is considered an effective stress
relieving heat treatment for carbon steel.

What will be the operating temperature of the system? That would determine my level of concern with the holding time.
Thank you for your reply.
The fluid design temperature is 50C.
We have electrical tracing + insulation to keep the temperature at this level.
 