I apply stl6 HFO with PTa on f6a material.
After machining the weld surface, there is no problem. weld surface checked with UT and liquid penetrant method
but after 3-4 days the all weld disbond from surface or seen big cracks.
do you have any suggest.
 
Replies continue below

Recommended for you

stl6?
HFO?
PTa?
f6a?

contamination?
residual stresses?

a picture or two (directly embedded not linked) might help
 
Thickness?
Code?
General dimensions?

Regards
 
After welding prior to any machining must be done penetrant , radiographic , then repeat
After machining then penetrant radiographic, and UT. Depending on the calibration method and the calibration defect UT will or could not detect slight subsurface defects. Most likely but not definitely
The grain structure change to fast and distorted.
Causing cracks. Was there a post weld stress relief. PWHT. Were the parts pre heated, was the recipe for gas purging was correctly processed.
Was there weld and mfg engineer review.
 
Surface texture?
Preheat?
Have you tried various deposition settings?
You are not using HVOF?
How thick of a layer and what contours?

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, consulting work welcomed
 
The condition of material ? And type ?
Is it annealed or core harden ,what percentage of carbon. Op can't answer the questions
 
Base metal designations that I'm not familiar with, likewise, I'm not familiar with the filler metal designation.

Best regards - Al
 