G... As You suspected... AND this is highly non-standard.
The form block for rubber-press hydroforming in sheet-metal 2024-T3 temper will have to include significant allowance for 'spring-back'**... which means a 90-Deg finished bend-angle will need to be bent to a substantially higher angle... unlike forming in the 'w' temper. Incorporating one-or-more joggles, at the same time, might not be feasible or practical on one form-block. [**I don't have spring-back tables handy, this PM]
The only-way I see this 'working' is a different approach... finger-break-form the part axially... then joggle-form transverse, afterwards... but even this seems overly complex/sketchy.
I am deeply curious as to 'why' You aren't forming in the O-> SHT-> W-> form-> age-to -T42 sequence?
NOTE.
A 'few tricks-of-the-trade' about heavy forming or stretch-forming in -T3 temper...
Ensure sheet metal is clean and free of surface scratches/gouges/etc
Deburr/radius all edges to prevent forming cracks.
Use aqueous forming lubricant [soap?] to minimize drag.
Immediately after forming, age HT to -T62 [I don't think -T81 applies after heavy forming] for stress relief and 'stability'.
Possibility of the appearance of 'Ludder's lines' is very real and may/may-not present a problem.
Regards, Wil Taylor
o Trust - But Verify!
o We believe to be true what we prefer to be true. [Unknown]
o For those who believe, no proof is required; for those who cannot believe, no proof is possible. [variation,Stuart Chase]
o Unfortunately, in science what You 'believe' is irrelevant. ["Orion", Homebuiltairplanes.com forum]