Eng-Tips is the largest forum for Engineering Professionals on the Internet.

Members share and learn making Eng-Tips Forums the best source of engineering information on the Internet!

  • Congratulations JStephen on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Dear all: what type of evaporatir should be used for caustic soda concentration up to 50%? Forced circulation or falling film? 4

Status
Not open for further replies.

Librianus

Chemical
Joined
Feb 28, 2025
Messages
6
Dear all
What tupe of evaporator should be used for caustic soda concentration up to 50%?
What construction materials should be used?
 
Solution
Material should be Nickel, based on my experience. Regarding operation, should be forced circulation due to the viscosity of caustic at high concentration.
Check physical properties of caustic solution. Pierre
There are a number of people out there with experience building these.
Steam heated.
There are only two material options, Ni200 or 26-1S (E-Brite) superferritic SS.
 
Material should be Nickel, based on my experience. Regarding operation, should be forced circulation due to the viscosity of caustic at high concentration.
Check physical properties of caustic solution. Pierre
 
Last edited:
Solution
Falling films could be considered as well or forced circulation is better?
 
There is a detailed discussion on this topic in Perry Chem Engg Handbook, chapter on heat transfer equipment , subsection on Evaporators.
 
Another resource:
You may want to contact them, both GEA and Alfa Laval
Pierre
 
Thank you so much, Pierre!
In my case, I need to project / specify a tubular unit.
 
I believe that Graham Mfg also makes these.
I have made a lot of E-Brite for this service, and have seen tubes with more than 40 years of service.
The issue with Ni200 is that it will erode from the excess salt in the solution.
 