Crevice corrosion in 316L threaded fitting

isakleivsson

Mechanical
Joined
Jun 5, 2025
Messages
3
Hi,
We har experiencing crevice corrosion on some threaded fittings, so looking for any guidance in troubleshooting and solving the problem. New here, not sure whether to add a bunch of photos along with this or not.

The equipment is 316L thin wall (2-3mm) piping that has 316L threaded check-valves connected on a 1.5" BSPT nipple, operated at 10barG. The threads are sealed with a combination of Teflon tape and Loctite 577. The piping is the distribution of a cleaning system that delivers sea water, detergent and desinfectant (see specs below) to various nozzles on some equipment that is placed on deck of fish carrying ships. This is in use a few hours a day intermittently, and detergent and ozone are for short periods in these cycles. The pitting is significant, but not yet through the thicker wall of the check valve. We became aware of this as some piping was dissasembled due to improper weld procedure that also caused pitting on the boundary of internal "sugaring" and caused a leak. It has been in service for about a year, but we do not know the number of washing cycles. On average probably used once a week.

The crevice corrosion is occuring on a number (not all) of the check valves, about 1/2 thread from the tip of the nipple (probably at the end of the starting thread chamfer). It is not at the bottom (with respect to gravity), the nipples are not welded on in a specific rotation with the respect to the threads. None of the nipples have any pitting on this or other parts of their thread. The orientation of the check valve is horizontal, and there is inner geometry that catches some liquid regardless of draining procedure (height difference in male/female threads, check valve seat etc). The piping is acid passivated, but the check valve does not appear to be (at least not in the same way, it has shiny threads). There is a few threaded adapters with pitting on the 60deg cone hose connections that are after the check valve.

Detergent (others use similar ones)
- pH 13 NaOH mixture. Safety sheet says <1% NaOH in the concentrate. mixed 2-3% in seawater to be 11 pH before it enters our piping.

Desinfection
- Mix of Hydrogen Peroxide (20-25%), Acetic acid (10-15%) and peracetic acid (~5%). Mixed 1% in seawater before it enters our piping.

The system runs a spray cycle (seawater), a detergent cycle, a rinse cycle (seawater), desinfection cycle and a final rinse cycle (seawater). Some likely deviate from procedure and do not use the final seawater rinse. The seawater is filter and UV-treated, but according to some accounts a bacteria test comes back positive if the final seawater rinse is performed.

The questions I have:
- Is the seawater rinse cycle critical? Seems from other forum posts seawater (especially stagnant) has no problem corroding 316L in crevices like these.
- Is it possible to reason to or to test whether the crevice corrosion is happening during the washing cycle or in the stagnant, after/between cycle?
- Will orienting this in a less horizontal way that drains more of the water drastically change the outcome, or is the amount of water/liquid that is going to be "stuck" in the threads going to do this regardless?
- Cathodic protection. Will installing a sacrificial cathode in the piping system have any effect on this? It will only be possible to add one for the bulk of the piping, so once it is drained wont each remnant liquid be unaffected? There are zinc anodes in other parts of our equipment, which are filled with seawater during use, but are not in any way in a liquid connection with this pipe system.
- Would passivating the check valve have a significant effect.
- Would a different joint type be less prone? I.e. if the check valve is flanged with gasket.

Any other tips/input is appreciated. Seems a "sealing" the threads option is possible, but from other forum posts also not guaranteed in any way.
 
Chlorides are trouble with 316 SS. If you're draining the pipe the remaining water with it's low chloride concentration will become super concentrated as the water evaporates and attack the SS. Consider blowing hot air through the piping after flushing for rapid drying.

Threaded connection will always be susceptible to crevice corrosion. Sealants can't solve that as there will be crevice corrosion at the toe of the sealant. BUT, you can reduce this effect by using ONLY the 577. You need to trust in your sealant and not come up with your own concoctions. Also PTFE tape is one of the worst for causing crevice corrosion. I don't have specific experience about the suitability of 577 for acids but I do know that that it works very well in seawater allocations.

It's good to think of anodic protection as being line of sight, while this may not be exactly true, anodes don't protect well around corners. Piping has too many corners.
 
Last edited:
1. As sea-water rinse cycle given in procedure, no point in deviating from it.
2. There is a basic difference between crevice and pitting corrosion. As per you, since it is crevice corrosion, so removing the crevice(s) is primary. Once there is a crevice, corrosion would occur, maybe at different rates during different cycles of operation, but this is not so relevant.
3. Refer point no. 2, removal of crevice(s) is primary.
4, 5 & 6. Painting is more appropriate.
 
Sea water is not sterile, so why would you rinse with it? If you are using UV to sterilize the rinse water, your testing is showing that not to be effective.
 
Are the valves made from castings or wrought material?
If castings they are likely not annealed properly.
You really should go to an all welded system.
And at that point also go to a better alloy.
the most cost effective option is likely 2205
 
As noted by @TugboatEng, 316 isn't a good choice where there are chlorides. Apparently the combination of chlorides + acid increases the susceptibility to crevice corrosion.

The alternating exposures to acid and basic solutions might be mucking up the passive layer by selectively leaching out Cr and Mo, increasing Fe in what's left behind. This is apparently temperature dependent.
 
The fact that this line is not used consciously makes things worse.
As it it sits some water will evaporate and this will concentrate the impurities.
 
Thanks for the replies!

@TugboatEng we will try to skip the PTFE. It was a tradesman's fix to a series of fittings that we had a problem sealing with only 577 (there was also a weather/curing issue), so Im sure we can solve those other issues given more necessity. It was apparent on the nipples (where the PTFE tape was still stuck) that the ones with "loose strings" of tape at the tip had the most rust-color (from the valves). Unfortunately the valves were disassembled before the location of each was noted. Will also look into the availability of a drying cycle. We have on some (maybe all) an air blowing cycle to help aid the draining, but I doubt there is any temperature control on it.

@Dhurjati Sen a problem of the customer is always right, so when they have trouble passing inspection they will rutinely make exceptions to the procedure if that helps them. We have however not been very pressing on the absolute necessity of the procedure (as we don't really have any lifetime data/experience with similar equipment until this point), so likely something we could make a demand for warranty eligebility in the future. We still need to gather more user data on who is or isnt following procedure to see if it will happen regardless, as long as either the chemicals or seawater could be the culprit.

@Compositepro the issues with sterilization is with one or a few of the customers, so need to verify what exactly their problem is as the info has become second and third hand at this point. The UV equipment they have on these vessels should in theory be sufficient.

@EdStainless the valves are a cast material. I'll look for alternative materials, but I'm guessing you are implying to change all parts of the system, and not just the problematic parts? Our supply chain (in Norway) is very 304 or 316 specific, so might take some doing. Would a passivating step on the valve make any difference? This is something we can easily apply. Side note, I have seen on occasion a "burned" look on some parts of the threads of parts that go through this step, seems to me something that could promote corrosion if in an exposed place. Something we should be careful of?


Some of the vessels have freshwater as a rinsing option (from a reverse osmosis system). Given the crevice nature of limited flow, even though it might not "rinse out" the contents in the crevice, there at least would be less chlorides to keep the reaction going in the water that is inevitably remaining?
 
You need to apply sealant to every thread. Tradesmen will typically leave the first two threads uncoated to prevent contamination. In your case, preventing crevices and galling are your #1 and 2 priorities so every male thread needs to be coated.
 
Are you kidding me? 2205 is very common in Europe.
It is even displacing 316 in most chemical process applications.
2205 costs a bit more but the prices are more stable (low Ni content), the material is much higher strength, and it has superior corrosion resistance in most applications.

I am guessing that your valves are not even annealed.
Changing those to 2205 might help, but eventually the threads of the 316 will crevice corrode and pit through wall.
I am with the comments to drop the tape and only use sealant.
But this needs to be uniform and controlled.
 
Ok noted. No application of sealant on the female thread?

@EdStainless definitely, just saying none of our current suppliers list these same type (or similar) check valves in any other material than 316. I will have our purchaser get in touch to see if they can source them though.

Follow up on the drying suggestion @TugboatEng. Does this need to be to the point where all liquid has evaporated, even from within the thread? Its unclear to me how/where the corrosion cell exist in this case of the threads, i.e. is it within different points in the thread or between the liquid most trapped in the thread and the liquid outside touching a larger surface? Maybe not possible to generalize either.
 
No, the female threas should not be coated.

Yes, drying needs to be complete. Any remaining moisture will be super concentrated.

The liquid pulls itself into the threads by capillary action. You need to trust your sealant to keep the liquid out of the threads. Most tradesmen are taught to not apply sealant to the first two threads. I think you'll find this is the region most of your crevice corrosion is occurring in which is why I recommend coating 100% of the male thread.,.
 
With crevice corrosion the tighter the crevice the worse the conditions.
Because pipe threads are tapered and truncated there will always be gaps.
This is why coating 100% of the male threads is a good method.
If you are going to dry I would suggest a short flush with pure water before drying.
And yes they need to be real dry.
 