A slab was poured in July 2012 on granular A materials. The granular 'A' materials was compacted to a 98%. The saw joints were placed at a distance of 10' 6". The average measured thickness of the slab was 6". Approximately after 8 months of the pour the cracks appeared on the concrete slab. The thickness of the cracks was measured between 0.5 mm to 1.5mm. The depth of the crack was around 2/3 depth of the slab. The designed strength of the concrete was 3600 PSI @ 28 day. The strength of the concrete core samples tested was 6100 PSI. The cracks appears to be a drying shrinkage cracks. During placement of the concrete the water was added in some of the concrete trucks prior to placement.
What factors causes concrete to crack? Is the higher strength of the concrete is one of them?
Please provide some comments on various causes for cracking.
What factors causes concrete to crack? Is the higher strength of the concrete is one of them?
Please provide some comments on various causes for cracking.