What would be a good corrosion resistant stainless steel to be used over 800C in an air / steam environment?

Structural strength is not of primary importance as pressures wont be going over 8 bar.

Would martensitic have any advantages over austenitic?

Thanks

 
Replies continue below

Recommended for you

Forgot to mention.

Application is steam piping.

Also cost is an issue.

Thanks
 
There are no martensitic grades suitable use at 800 C. Type 310 austenitic stainless is a common high temperature grade.
 
No, martensitic steels have no advantage because of softening and creep strength above 1200 deg F or 650 deg C. At 800 deg C you are going to be limited to Nickel-base alloys, like 800H. I would refer you to ASME B&PV Code, Section II, Part D and search for alloys permitted to 1500 deg F or 820 deg C.
 
I found my copy of B31.1 Power Piping Code and for 1500 deg F service, you can use TP 304H pipe material under ASTM A 376. See Appendix A-8. I would strongly recommend you follow B31.1 for piping. Other stainless steel high temperature pipe grades are not necessarily listed.
 