Corrosion(?) on stainless at a waste water plant

Big_Daddy

Mechanical
Joined
Apr 10, 2025
Messages
6
We are a fabrication company that specializes in waste water treatment plants. We recently completed a project in Phoenix, AZ where we replaced two drum screens at one of the largest waste water facilities in the country. These drum screens are not supposed to be on the sanitary (sewage) side, but rather on the run-off (storm drain) side.

The replacement screens and covers were set in place November of last year. In March of this year, they were tested in dry-bed conditions (the water ways were empty) but we did run the clean out spray nozzles for quite a while. The plant was also charged with running the screens and nozzles weekly until full operation is in play (October of this year). These units are exposed to the elements and are not contained within any facility.

We were able to save the original interior drum skeleton. This drum is made of carbon steel and is coated with Dura-Plate (Sherwin Williams) and was Holiday tested for proper coating thickness and coverage. We did have to add new 304 stainless screens and 304 stainless steel screen plates to the drum. We used 316 stainless hardware to connect everything.

We also built new 304 stainless steel covers, along with all 304 stainless piping when the units were installed.

The plant has now tested the units with the water ways full as if in actiive opoeratioon (remember, these are not suposed to go on line until October of this year). I have no idea how long they tested or how many times they have tested, but they have sent us these pictures:

This first picture is the outside face of the actual drum that sits inside the cover. Remember, the drum skeleton is carbon steel coated with Durua-Plate and the outer plates and screen are 304 stainless while the hardware is 316 stainless. Notice that the screen material does not look to have this discoloration. What is causing this and the stuff that looks like somebody sprayed something on the outer cover?


SCREEN PANELS.jpg

We have a theory and I will disclose that after we get some comments related to what this may be.

This next picture is of a 304 braided stainless steel flexible hose. This will be changed out to hard pipe (against my urge to leave as is):
BRAIDED LINE.jpg
Note there is more staining on the catch trough in the background.

These next two pictures are the welds on the 304 stainless piping: (ignore the fact that the one flange is missing nuts. I have already addressed this)
PIPE WELDS.jpg BLACK WELDS.jpg

The contractor in charge of this project is looking for answers before they turn it back over to the city. I am hoping that someone can help me analyze this to see if there is anything that can be done to have prevented this (using the materials listed) and if there is anything that can be done to prevent it happening any further.

Again, when we tested the system (early March), these did not look like this. A month later and this is what we have. So, we feel pretty sure that this has something to do with the water they are running in and something to do with the H2S gasses these are subjected to. We also feel, short of additional coatings or alternate materials, that there is nothing we could have to done to prevent the corrosion on the screen parts (the welds could just be where the welds weren't cleaned or passivated).

Any input is greatly appreciated.
 
We are a fabrication company that specializes in waste water treatment plants. We recently completed a project in Phoenix, AZ where we replaced two drum screens at one of the largest waste water facilities in the country. These drum screens are not supposed to be on the sanitary (sewage) side, but rather on the run-off (storm drain) side.

The replacement screens and covers were set in place November of last year. In March of this year, they were tested in dry-bed conditions (the water ways were empty) but we did run the clean out spray nozzles for quite a while. The plant was also charged with running the screens and nozzles weekly until full operation is in play (October of this year). These units are exposed to the elements and are not contained within any facility.

We were able to save the original interior drum skeleton. This drum is made of carbon steel and is coated with Dura-Plate (Sherwin Williams) and was Holiday tested for proper coating thickness and coverage. We did have to add new 304 stainless screens and 304 stainless steel screen plates to the drum. We used 316 stainless hardware to connect everything.

We also built new 304 stainless steel covers, along with all 304 stainless piping when the units were installed.

The plant has now tested the units with the water ways full as if in actiive opoeratioon (remember, these are not suposed to go on line until October of this year). I have no idea how long they tested or how many times they have tested, but they have sent us these pictures:

This first picture is the outside face of the actual drum that sits inside the cover. Remember, the drum skeleton is carbon steel coated with Durua-Plate and the outer plates and screen are 304 stainless while the hardware is 316 stainless. Notice that the screen material does not look to have this discoloration. What is causing this and the stuff that looks like somebody sprayed something on the outer cover?


View attachment 8112

We have a theory and I will disclose that after we get some comments related to what this may be.

This next picture is of a 304 braided stainless steel flexible hose. This will be changed out to hard pipe (against my urge to leave as is):
View attachment 8113
Note there is more staining on the catch trough in the background.

These next two pictures are the welds on the 304 stainless piping: (ignore the fact that the one flange is missing nuts. I have already addressed this)
View attachment 8114 View attachment 8115

The contractor in charge of this project is looking for answers before they turn it back over to the city. I am hoping that someone can help me analyze this to see if there is anything that can be done to have prevented this (using the materials listed) and if there is anything that can be done to prevent it happening any further.

Again, when we tested the system (early March), these did not look like this. A month later and this is what we have. So, we feel pretty sure that this has something to do with the water they are running in and something to do with the H2S gasses these are subjected to. We also feel, short of additional coatings or alternate materials, that there is nothing we could have to done to prevent the corrosion on the screen parts (the welds could just be where the welds weren't cleaned or passivated).

Any input is greatly appreciated.
First question
Was there passivation, and proper packaging
, vacuum sealed
Or similar.

Second question
Was there any heat treat involved as Ed stainless any post weld heat treat has to be low as possible.
Any solution anneal , and any fabrication, post NDT Is done to verify no intergrannual attack.
Or other indications.
I would recommend a failure analysis, Send sample out a Matlab to apply some type of analysis of the chemicals on the SS, and of the part grain structure. High power and sem.
Then one by one remove what it is not. To zero down what it is. There maybe additional coating
Required.
PS once corrosion starts its hard to remove. So the fix will be to prevent it.
 
If this is all superficial then there are ways to clean it up.
Clean it with fresh abrasive and then wipe down with pickling paste and then wash well.
But the bottom line is that 304 is barely corrosion resistant.
This is why duplex SS has become so popular.
My hunch is that they have gotten it wet, then let it set and dry, then wet again and so on.
This will concentrate impurities on the surface.
It might just be iron deposited on the surface or it could be active corrosion of the SS.
But it looks like surface contamination and perhaps some heat tint next to the welds from poor shielding.
 
Last edited:
Well that's a good point , however looking at the pictures , looked deep to me but looks could be deceiving.
The welds visually look terrible.

OP
Can a fitter take spot Scotch bright. And or light sanding. Take before and after picture.
 
As I recall, Pheonix water is somewhat high in chlorides. Some of the photos look like iron contamination from improper cleaning but only so much can be gleaned from the photos.
 
Sorry for the late respnses here. I appreciate everyoine's feedback.

Our fab shop deals mostly with carbon steel. We have a neighboring fabricator that is all stainless - so we farmed the stainless fabrication off to them. So, being honest, I don't know that I can answer the passivation questions without inquiring with the neighbor. I will have to do this and then go from there.

As far as having the fitter go out with scotch brite...we will have to send our guy back out there. We are located in Georgia.
 
If it is a big deal to go out there then make sure to do it all.
Take new abrasive scotchbite pads, pickling paste (from a welding supply store) and all of the PPE.
Trust me, this paste will take you skin off down to the bone in seconds, don't mess around.
And then wash it all down very well.
Any places showing this much surface rust this soon are at risk.
Even if there is no pitting now the surface rust will accelerate future pitting corrosion.
 
EdStainless - I truly appreciate your input on this. You have given me the ammunition (for lack of beter words) to play our case on.

Just so I am not leaving anyone out, I appreciate everyone's input as well. I have taken everything that has been siad into consideration. I will be coupling this with what I know about the system in place at the WWTP and puting together a respnse email this afternoon.
 
If this is all superficial then there are ways to clean it up.
Clean it with fresh abrasive and then wipe down with pickling paste and then wash well.
But the bottom line is that 304 is barely corrosion resistant.
This is why duplex SS has become so popular.
My hunch is that they have gotten it wet, then let it set and dry, then wet again and so on.
This will concentrate impurities on the surface.
It might just be iron deposited on the surface or it could be active corrosion of the SS.
But it looks like surface contamination and perhaps some heat tint next to the welds from poor shielding.
Agreed.
304 stainless steel is sufficient for most everyday applications, especially in dry or mildly corrosive environments. However, in the presence of chloride ions (such as salt, cleaning agents, or coastal air) or acidic conditions, 304 is prone to pitting corrosion and intergranular attack.
In seawater environments, it's better to use stainless steels with higher corrosion resistance, such as:
316L: Contains ~2% molybdenum for improved resistance to chlorides, but may still pit in actual seawater.
2205 duplex stainless steel: With a PREN over 35, it offers excellent resistance to pitting and crevice corrosion in marine environments at a more economical cost.
2507 super duplex: Has a PREN above 40 and is highly resistant to aggressive seawater corrosion, ideal for desalination plants and offshore platforms.
904L and AL-6XN: High in nickel and molybdenum, designed for extreme chloride or acidic environments—very corrosion-resistant, but more expensive.
 
EdStainless - I truly appreciate your input on this. You have given me the ammunition (for lack of beter words) to play our case on.

Just so I am not leaving anyone out, I appreciate everyone's input as well. I have taken everything that has been siad into consideration. I will be coupling this with what I know about the system in place at the WWTP and puting together a respnse email this afternoon.
You must have got to the bottom of the issue by now.
It would be nice if you share the findings in the forum.
Even if no action was taken as the corrosion seemed superficial, stating it would enrich us
 