Do you see any big issues having a big bronze tank and threading galvanized carbon steel on it?
Room temperatures and the environment is sea water.

Thanks,

Herc.
 
Can you provide the expected duration for immersion? Expected lifetime?
 
Yes, I see a number of issues.
Dealloying of the bronze is probably going to happen.
There is also the risk of galvanic corrosion of the steel adjacent to the bronze.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
Are there any diagrams I can take a look at to see corrosion rate for this setup?
 
Unless you install dielectric unions to isolate the bronze from the zinc-coated steel, you will have a 1.5 volt, high current battery actively dissolving away the galvanized pipe the whole time the thing is in service. Even in a situation where the seawater is deoxygenated by virtue of being in a totally closed loop, I'd be concerned.

As to service life: that depends on lots of stuff. It might last a while, but it's still bad practice. It would be bad practice in fresh water services without corrosion inhibitors, and it certainly is bad practice in seawater.

 
I'm with moltenmetal. A galvanic difference that high in seawater will lead to rapid corrosion.
 
Herc,

You might be able to get 3 years out of this type of arrangement, if a number of things are optimized (coating, preload/stress in threads, etc). The technical points that everyone else noted are the relevant items of concern. I wouldn't even consider using this type of arrangement, and strongly encourage you to find another solution that doesn't have such inherent corrosion issues.
 