Hi, we have a valve for which all the pressure bearing weldments have their WPS/WPQR and qualified welders. But we have a bronze cladding just to lower the friciton. Is not a pressure bearing, nor under stress. Do I need a the same process as for the pressure bearing weldments?

Best regards
 
Replies continue below

Recommended for you

If it is a pressure retaining part, then yes, the welding procedure needs qualification to Section IX (QW-216 Hard-Facing Weld Metal Overlay).
Likewise your welders require qualification to QW-382 Hard-Facing Weld Metal Overlay (Wear Resistant). No qualification is unlimited in scope.
p.s., there is no such thing as a non-load carrying weld.

"If you don't have time to do the job right the first time, when are you going to find time to repair it?"
 
Thanks for you help Will have to take a look.

Best regards
 