Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations JStephen on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Bearing Babbitt Melting Temperature 1

Status
Not open for further replies.

jamesjm

Mechanical
Joined
Jul 8, 2005
Messages
12
Location
US
On average, what is the melting temperature of the babbitt on a journal or tilt-pad thrust bearing?
 
I have never measured it. It may vary depending on the particular babbit metal used. But I have always used 350 °F as the expected melting temperature. However, I would never deliberately run a babbit bearing at an operating temperature above 250 °F.
 
The melting point for common babbit is 462°F. This is for the lead/tin and tin/lead babbits.
 
The common tin-base and lead-base babbits are specified in ASTM B23. For high performance rotating equipment,tin-base is the choice, and the lead should be specified as low as possible.

For ASTM B23, Babbit types /melting temperature deg F
1 433
3 464
4 363
5 358
7 464
10 468
11 471
12 473
16 471
19 462
 