Vdubb98

Mechanical
Jan 4, 2008
2
I'm writing a weld procedure to tack a Nut (SA-193 gr. B7) to a valve indicator body. I have the P-number for the valve body but there is no p-number listed for SA-193 gr. B7. Can I do an equivalency for SA-193 based on chemical composition and if so what is the criteria? Thank you very much for any assistance you can provide!

Jake, E.I.T.
 
Replies continue below

Recommended for you

There is no P-No. for the A-193 B7 bolt and you cannot equate a P No. to it. Also the B7 material may include a number of AISI low alloy steels such as AISI 4140. Please note that A-193 is a bolting specification - not a nut specification.

 
Vdubb98, when welding -B7 studs to -2H nuts for low risk situations, such as making a jackbolt or something, I instruct the shop to "weld it like it's a low-chrome". They generally NDE the completed weld.

BTW, we had a fairly serious injury sometime back because the shop had taken it upon itself to weld two -B7 studs together end-to-end to make a longer one for drawing some parts together or something like that. It let go when no-one was ready. Welding studs together is not permitted these days.

Regards,

Mike
 
Vdubb98;
I would recommend an ASTM A 194 2H carbon steel nut (P-No 1) to tack weld on the valve indicator body, versus a low alloy grade nut. If you decide to use a stud instead of a nut, go with a carbon steel grade stud versus Grade B7.
 
Thank you all very much for your excellent replies. Your input was very helpful!!