May 5, 2015 #1 Qual7Eng Mechanical Joined Apr 20, 2014 Messages 21 Location IN Hi, great day, Anyone, please help me out for an welding electrode for Casting of ASTM A352 Gr.LC2-1? UTS:725-895 Mpa YS:550 Mpa Impact @ -73DegC 41J(Avg)
Hi, great day, Anyone, please help me out for an welding electrode for Casting of ASTM A352 Gr.LC2-1? UTS:725-895 Mpa YS:550 Mpa Impact @ -73DegC 41J(Avg)
May 5, 2015 #2 metengr Materials Joined Oct 2, 2003 Messages 15,478 Location US E10018M for the SMAW process. The LC2-1 composition for SA 352 contains 2.5-3.5% Ni, so you need to locate a filler metal or wire with a nominal composition of Ni, for starters, also with Cr and Mo for strength. Upvote 0 Downvote
E10018M for the SMAW process. The LC2-1 composition for SA 352 contains 2.5-3.5% Ni, so you need to locate a filler metal or wire with a nominal composition of Ni, for starters, also with Cr and Mo for strength.
May 5, 2015 #3 weldstan Materials Joined Jun 24, 2011 Messages 2,809 Location US ER100S-1 or ER110S-1 would also work for you. Upvote 0 Downvote
May 6, 2015 Thread starter #4 Qual7Eng Mechanical Joined Apr 20, 2014 Messages 21 Location IN @metengr ,am afraid whether E10018M could bear impact @ -73DegC? Upvote 0 Downvote
May 6, 2015 #5 metengr Materials Joined Oct 2, 2003 Messages 15,478 Location US You try and qualify the WPS. If not, try E8018 C2, under matching in strength but is stated to meet 27 J at –75°C. Upvote 0 Downvote
You try and qualify the WPS. If not, try E8018 C2, under matching in strength but is stated to meet 27 J at –75°C.