Dear All,
My Question is : If a welder has done performance qualification for SMAW using E-7018, would also qualified for E8018 ?
Note : other variables are unchanged
 
Replies continue below

Recommended for you

Yes, assuming no other change from E7018 to E8018 (see ASME BPV Section IX Table QW 353), and as qualified with/without backing.

See ASME BPV Section IX, QW 404.15,and Tables QW-432 and QW-433.
 
First, please review Section IX, QW-353, now look at filler metals, either a change in F-No or thickness deposited are essential variables. You can figure this out.
 
For both electrodes the type of covering is Low-hydrogen potassium, iron powder (Designator 8). Electrodes with this covering type are assigned to F-No. 4 (see Tables QW-432).
Acc. to Table QW-353 with reference to QW-404.15 your welder is also qualified for E8018.

Regards - Juergen
 