My Question is : If a welder has done performance qualification for SMAW using E-7018, would also qualified for E8018 ?
Note : other variables are unchanged
First, please review Section IX, QW-353, now look at filler metals, either a change in F-No or thickness deposited are essential variables. You can figure this out.
For both electrodes the type of covering is Low-hydrogen potassium, iron powder (Designator 8). Electrodes with this covering type are assigned to F-No. 4 (see Tables QW-432).
Acc. to Table QW-353 with reference to QW-404.15 your welder is also qualified for E8018.