Dear all,

It is my company's standard practice to limit the use of 1.25Cr-0.5Mo material for pressure vessels with applications at minimum temperature above -18°C, due to the difficulties that vessel manufacturers have reaching impact test energies with this material and welded assemblies at such low temperature.

ASME VIII div.1 section UCS-66 and figure UCS-66 provide :
- note (2)(b) : "Curve B applies to [except for cast steels] all materials of curve A if produced to fine grain practice and normalized which are not listed in curves C and D below"
- note (2)(c) "Curve B applies to all pipe, fittings, forgings and tubing not listed in curves C and D"

ASME B31.3 section 323.2.2 and table 323.2.2 provide :
with MDMT > -29°C : no impact test requirements for base metal, weld metal and heat affected zone

I thus have the following question :
Why does the ASME BPVC and ASME B31.3 cover the use of 1.25Cr-0.5Mo material without impact test down to -29°C for pressure vessels and piping sytstems, knowing that 1.25Cr0.5Mo material is unable of sustaining temperatures below -18°C ?

thank you in advance

regards
 
Because the problem is that when the stress tables were developed, the metal temperature listed was for allowable stress only and not notch toughness. There is a movement within BPV II to revise the metal temperature in Part D as being only applicable to stress lines and not notch toughness.
 
35 years ago we were able to obtain this material impact tested at -20F with 30 ft-lbs min absorbed energy. Base metal thickness was over 2" thick. Client was applying heavy wall hydrocracker technology to 2" and over 1 1/4 Cr applications even though the MDMT was >> -20F.
 
thanks for your answers
I understands that the stress related mechanics (ASME stress tables) allow for the use of 1.25Cr-0.5Mo material at low temperature (above -29°C without impact test, below -29°C with impact test), but also that this material cannot pass impact test at such a low temperatures.

Then I will limit the use of 1.25Cr-0.5Mo to MDMT above -18°C, and ask for impact tests at MDMT for base material and welding procedure coupons.

In your opinion and because the impact toughness of 1.25Cr-0.5Mo is not well decribed in ASME, what do you think would be the limit temperature above which impact testing is not necessary for base metal and welding procedure ? ASME B31.3 says -29°C but i think i cannot use this value. On which normative document / construction code can I base the definition of that temperature limit?

thx & regards


 
Chumpes;
That was my point earlier in the thread. The metal temperatures stated in ASME Section II, Part D do NOT apply to impact testing only stress lines. Over the years, user's have assumed that the reference to -20 deg F to 100 deg F metal temperature also applied to impact testing exemption.

If this material is intended to be used below room temperature (non-boiler), impact testing should be performed rather than assuming -29 deg C.
 
Hi Chumpes;

You may take a look at API-RP-934C & 934E as additional resource.Both of these RPs are on 11/4CR-1/2Mo Steel Pressure Vessels for hydroprocessing services.The toughness requirements are as follows:-
The minimum CVN impact values shall be 40 ft-lbs(54 Joules) average of three specimens at 0 °F (–18 °C) and 20 ft-lbs (27 Joules) minimum for a single specimen
at 0 °F (–18 °C).
Charpy impact as stated above would be difficult to meet @ -29 Deg C.

Looking at the requirements of Table 323.2.2 & Fig. 323.2.2A, the requirements are more for C-Mn Steel.Possibly 1.25Cr-1Mo steel does not fit in to these curves.

Thanks.

Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299
 
Status
Not open for further replies.

Part and Inventory Search

Sponsor

Back
Top