Hi all,

Does anyone know the reason for the impact test requirement changes in 2020? Specifically the minimum temperature requiring impact testing changing from -29C to -18C?

I can't find any commentary. I expect it to be based on some material science discoveries?

Thanks in advance,
Tiz
 
It would help if you noted specific clause or Table that has been revised. (or specific material)
 
Paras. 323.2.2, 323.3.1
 
Does the change align B31.3 with B31T?

Sorry - I don't have the 2020 Edition yet...
 
Hi TGS4.

Thanks for giving me a place to start looking! I don't have access to B31T but will try and get a copy.

Do you know if there is a way to find the 'basis' for the requirements. I.e. if B31.3 now aligns with B31T, why are the requirements different in the first place?

Thanks again
 
tiz99,
I started researching for you and this goes all the way back to 2015.
I have asked the original PM for clarification on the change.
There is also a proposal to include B31T in B31.3 some time in the future,
Cheers,
DD
 
Tiz,
This is an informal response I received.

As a rule contractors will use filler metals that have been impact tested at -29°C when impact testing is required, but there are a lot of materials where the filler metal specification does not specify any impact testing. Engineers routinely pick -29°C as the lowest service temperature, including for system use for steam. B3 and other Cr-Mo weld metal as-welded is like glass at -29°C, not quite so bad at -18°C, not that steam systems operate at -18°C.Cr-Mos are tough as hell if they get PWHT, but code permits them to be used as-welded.

The fix is as simple as specifying the lowest service temperature as -18°C unless you plan to use a system below that temperature.

Hope that helps,
Cheers,
DD
 