A contractor has specififed an "as rolled" steel for the shell plates of a storage tank they are building. Specifically it is EN10025: 2004 S275JR + AR.

I am not fully up to speed with this option and I'm wondering about any pitfalls compared to plain normalised or normalising rolled plate.
This is a welded fabrication and will also be stress relieved after fabrication. Perhaps increased distortion may be encountered?

Could anyone enlighten me? Thanks
 
DefenderJ
If the storage tank does not have a specified minimum design metal temperature (MDMT), the as-rolled plate will be acceptable. If there is a minimum design metal temperature due to location of installation, as-rolled plate may not have the necessary minimum specified impact energy requirement for service. You need to evaluate this before accepting the material.
 
Thanks metengr.
Have reviewed min design temperature and decided to specify normalised grades.
 
The normalizing in oil and gas industries is generally required from the following conditions.

1. At low temperature : to obtain the required/higher impact energy values at the MDMT. (see API 650, 4.2.8 to 4.2.10.)
2. At corrosion cracking environment : to minimize the risk of crack.
3. At heavy wall thickness : to keep the sound/higher mechanical properties. (see API 650, 4.2.1.4, ASTM A516, 5.2, etc.)

So the final decision depends on the MDMT, thickness, corrosion environment, and others (specs, codes, etc.).

Thomas Eun
 