hello there,
is there any difference in mechanical properties between API 5L X65 M&N&q or the are the same ?
also when i specify to the manufacturer M,Q or M
 
The required properties for each grade are the same, whatever be the delivery condition, since M is for thermomechanical rolled or formed, Q is for quenched and tempered and N is for normalized.
 
Amr Srag,

The delivery condition for PSL-1 pipe is at the option of the manufacturer, unless specified in the purchase order. For PSL-2 pipes, the delivery condition should be specified in the purchase order, as well as indicated in the grade name. See below for a difference of the two product specification levels.

Capture_gorfw1.jpg


"Thinking is the hardest work there is, which is probably the reason why so few engage in it."

-Henry Ford
 
I have been wondering the same thing. With the properties being required to be the same, why would I care to specify a delivery condition for PSL2? For my company's purposes, we indicate that any of the PSL2 delivery conditions are acceptable, and don't require a specific one, but I'm wondering if there are properties of the different delivery conditions not specified in API 5L that we should be aware of.

We are building gas compressors, so our scope is limited to piping of about 16" and less.
 
Thank you all very much for your answers, so as conclusion there is no selecting criteria for M,Q or N they are the same (only a method of manufacturer don't effect by any way the material properties and no method is better than other. thus, whether i specified in the pipeline data sheet M or Q they are the same ?
 
Not exactly:
As we mentioned before, the API grade refers to minimal yield stress required (SMYS), and there are an specific interval where yield strength and Ultimate tensile strength can belong to each grade, but, there are other properties like toughness (represented by CVN Energy or DWT), ductility (represented by elongation in tension test and shear fracture in impact test), where API only specifies minimal values for each grade and each one could be improved by different delivery condition and the user must be establish optimal levels based on the requirements of the engineering design for the specific pipeline.

Other properties like hardness will be different in each delivery condition, maybe higher in Quenched and tempered steel, and this property are important where you could have friction, erosion, impacts but shall be well controlled if there is probability of SSC or hydrogen damage by example.

The use of Q grades involves also the need for more controlled welding procedures, to avoid undesirable effects in each weld.

Finally, some studies try to establish relationships between microstructure (the microstructure is probably the main difference between each delivery condition) and corrosion resistance and how could be improved.

Summary: You must order M, N or Q grades when the engineering design for the specific pipeline demands it.
 
A last thing: you need specify N, M, Q..... If you need PSL2 pipe, since PSL 1 no requires.

When PSL1, when PSL2???
R. again: engineering design and... Maybe a rule of thumb: liquids at room temperature or moderately different, could be PSL1. Others services, PSL2.
 
thank you all, it was very helpful
 