24
I am in possession of some 2" xs API 5L X52 PSL 2 Hyundai the producing mill did not report the CVN results on the MTR.

I am being told that 4" and below does not have to show results on the MTR. But I would need to prove this to our customer.

Table 22 gives the requirements per size for reported results. But it starts at 4.5" O.D..

No where can I find within API 46th ED. PSL 2 where it states below 4" is non reportable??? Can one of you fine folks point me in a direction please?

As always, thanx in advance.

-=Fred=-

Vass Pipe API Line Pipe Industry Leader

People do what you inspect, not expect!
 
 https://files.engineering.com/getfile.aspx?folder=83d92793-6bbf-4db3-9155-e02cd89f58a8&file=Capture.JPG
Replies continue below

Recommended for you

Refer to note at the end of 10.2.3.3: "It is not necessary to CVN impact test combinations of specified outside diameter and specified wall thickness not covered by Table 22."
 
Been scouring the book for 2 days and did not see that!!!!

Thank you very much!