Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations MintJulep on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

AISI 321 SS, weld rod selection

Status
Not open for further replies.

darock

Electrical
Joined
Nov 16, 2005
Messages
2
Location
IE
Could someone confirm the correct weld rod selection for the welding together of AISI 321 SS clad (10 mm thick)
 
More information is needed.
Could you explain your joint detail and application?
 
Standard filler wire selection for plain 321 SS is 347.
However if you have stainless clad on carbon steel you need a complex procedure.
Weld first the carbon steel side without penetrating the stainless cladding.
Backgouge the carbon steel and butter the carbon steel surface of the joint with 309 or 312 filler metal.
Fill the gap with 347.

 