Jul 29, 2019 #1 mtnz Aerospace Joined Dec 4, 2018 Messages 21 Location US Hi Guys! I know 1144 is an oil quench material. I was just curious what happens if we air cool 1144? Would it be still hardened ? Thanks!
Hi Guys! I know 1144 is an oil quench material. I was just curious what happens if we air cool 1144? Would it be still hardened ? Thanks!
Jul 29, 2019 #2 EdStainless Materials Joined May 20, 2004 Messages 16,367 Location Waukesha WI USA Thin parts? Forced air? Might work. = = = = = = = = = = = = = = = = = = = = P.E. Metallurgy, Plymouth Tube Upvote 0 Downvote
Thin parts? Forced air? Might work. = = = = = = = = = = = = = = = = = = = = P.E. Metallurgy, Plymouth Tube
Jul 29, 2019 Thread starter #3 mtnz Aerospace Joined Dec 4, 2018 Messages 21 Location US 1.5" thick, 14" long pin ? Upvote 0 Downvote
Jul 29, 2019 #4 EdStainless Materials Joined May 20, 2004 Messages 16,367 Location Waukesha WI USA No chance at 1.5" diameter in air. Will it through harden even with an oil quench? = = = = = = = = = = = = = = = = = = = = P.E. Metallurgy, Plymouth Tube Upvote 0 Downvote
No chance at 1.5" diameter in air. Will it through harden even with an oil quench? = = = = = = = = = = = = = = = = = = = = P.E. Metallurgy, Plymouth Tube
Jul 29, 2019 Thread starter #5 mtnz Aerospace Joined Dec 4, 2018 Messages 21 Location US You mean it won't get hardened at all? Upvote 0 Downvote
Jul 29, 2019 #6 EdStainless Materials Joined May 20, 2004 Messages 16,367 Location Waukesha WI USA The outer surface will, but the properties through it will be lower, and maybe rather bad. If this pin is going to be loaded you might want to re-think your grade. = = = = = = = = = = = = = = = = = = = = P.E. Metallurgy, Plymouth Tube Upvote 0 Downvote
The outer surface will, but the properties through it will be lower, and maybe rather bad. If this pin is going to be loaded you might want to re-think your grade. = = = = = = = = = = = = = = = = = = = = P.E. Metallurgy, Plymouth Tube
Jul 29, 2019 Thread starter #7 mtnz Aerospace Joined Dec 4, 2018 Messages 21 Location US I don't need to thru harden the pin. I need to case harden it, so I believe it will work then ? Upvote 0 Downvote
Aug 15, 2019 #8 weldstan Materials Joined Jun 24, 2011 Messages 2,809 Location US Probably not; depends on the surface hardness and depth of hardness required. Upvote 0 Downvote
Aug 15, 2019 #9 weldstan Materials Joined Jun 24, 2011 Messages 2,809 Location US I assume you still wish to air cool. Upvote 0 Downvote
Aug 16, 2019 #10 Tmoose Mechanical Joined Apr 12, 2003 Messages 5,636 Location US Are you buying 1144, or "sress proof" ? Upvote 0 Downvote
Aug 19, 2019 #11 Guest 1144 should respond very much like 1045, a very common material for which there is an abundance of data. "Everyone is entitled to their own opinions, but they are not entitled to their own facts." Upvote 0 Downvote
1144 should respond very much like 1045, a very common material for which there is an abundance of data. "Everyone is entitled to their own opinions, but they are not entitled to their own facts."
Aug 20, 2019 #12 dbooker630 Materials Joined Apr 16, 2004 Messages 525 Location US You can expect hardness around 269 HBW (28 HRC) after air cool in this section size. Upvote 0 Downvote