Nov 17, 2010 #1 Dijor007 Mechanical Joined Nov 15, 2010 Messages 1 Location ES Hi, Whithout any specific service what are the restriction to made PWHT to A216WCB(pump casing) after welding nozzles. thks in advance
Hi, Whithout any specific service what are the restriction to made PWHT to A216WCB(pump casing) after welding nozzles. thks in advance
Nov 17, 2010 #2 metengr Materials Joined Oct 2, 2003 Messages 15,478 Location US If you have no Code of Construcction, follow good engineering practice - - 1" or greater weld deposit thickness, PWHT at 1100 deg F - 1 hour/inch of weld deposit thickness. Upvote 0 Downvote
If you have no Code of Construcction, follow good engineering practice - - 1" or greater weld deposit thickness, PWHT at 1100 deg F - 1 hour/inch of weld deposit thickness.