Good morning! I have done several 4130 procedures in the past, however I am having trouble with the mechanicals and testing on a thinner specimen.
Codes:
API 6A
DNV OS E101
ASME IX
NACE MR0175
I have tried using SMAW/FCAW/GMAW-spray.
Preheat: I have tried 400 & 600
SMAW: 10018 D2 (1/8")
GTAW Root: ER100S-G
I've had welders try welding wall->wall->middle fill all the way out.
*EDIT* PWHT 1190F @ 8 Hours and 1175F at 4 hours.
The biggest problem I am having is with the NACE hardness requirement of 250 Vickers in the HAZ. I've used propane torches for preheat and resistance ceramic blankets both which were wrapped in insulating material during and after welding to control heat loss. As far as I know the cooling rate has a big effect on the HAZ hardness.
Both tests I have tried were using a roll out on a piece of pipe. I could use some advice so I don't just keep trying to make something happen that may or may not work. It could just be something that I am missing.
Codes:
API 6A
DNV OS E101
ASME IX
NACE MR0175
I have tried using SMAW/FCAW/GMAW-spray.
Preheat: I have tried 400 & 600
SMAW: 10018 D2 (1/8")
GTAW Root: ER100S-G
I've had welders try welding wall->wall->middle fill all the way out.
*EDIT* PWHT 1190F @ 8 Hours and 1175F at 4 hours.
The biggest problem I am having is with the NACE hardness requirement of 250 Vickers in the HAZ. I've used propane torches for preheat and resistance ceramic blankets both which were wrapped in insulating material during and after welding to control heat loss. As far as I know the cooling rate has a big effect on the HAZ hardness.
Both tests I have tried were using a roll out on a piece of pipe. I could use some advice so I don't just keep trying to make something happen that may or may not work. It could just be something that I am missing.