My supplier is out of 260 Cartridge Brass - Hard Temper which is being used to manufacture flat washers. Can somebody advise me, if the half hard temper which is readily available be used as a replacement?

Thanks in advance!
 
Replies continue below

Recommended for you

Johnson_123 ,
In order to get an intelligent answer to that question, you would have to describe the loads the washer is subject to.
a softer washer may or may not be adequate.
B.E.

You are judged not by what you know, but by what you can do.
 
Johnson 123

BE CAUTIOUS: bearing [crushing] strength of a washer is an important mechanical feature. IF understrength [low yield/crush], then joint will likely loosen in-service!

Per MIL-HDBK-698, Table XXI...
Alloy 360 [KSI]...
Strain temper UTS TYS %El
H [<0.187 thick] 80 45 -ns-
1/2H [<0.50 thick] 57 25 7%

Regards, Wil Taylor

o Trust - But Verify!
o We believe to be true what we prefer to be true. [Unknown]
o For those who believe, no proof is required; for those who cannot believe, no proof is possible. [variation,Stuart Chase]
o Unfortunately, in science what You 'believe' is irrelevant. ["Orion", Homebuiltairplanes.com forum]
 
Status
Not open for further replies.

Part and Inventory Search

Sponsor