Hello,

I need to create a rubber sheeting from HA latex. It must have a high resilience, tearing resistance, flex fatique life and rebound elasticity. Thus, I chose a conventional postvulcanization with sulfur, ZDEC, zinc oxide and stearic acid

However, I have some problems finding the right combination of the beforementioned ingredients. Does anyone have basic formularies of what's typically used for latex products such as surgical tubing, condoms etc?
 
Replies continue below

Recommended for you

THF - here is an old condom formulation I have in my records, which should go some way to helping you. It is based on HA latex and uses emulsions and dispersions for the other ingredients.

60% LA NR latex 167.0 parts
10% potassium hydroxide 2.0 parts
20% potassium laurate 0.5 parts
50% sulfur 1.8 parts
50% ZDBC 1.0 part
50% ZMBT 2.5 parts
50% non-toxic, non-staining antioxidant 1.0 part
(phenolic type)
Water 24.0 parts
 
Thanks, GrahamBennett. I must do with ZDEC only for the moment, but will gladly try your formulation if my further experiments fail.
 