Hi all,
We have ordered Side Pocket Mandrels (Quantity: 50 No’s) with monogram & testing to API 1G1 V1 F2.
As per API 19G1, for F2 grade, 5% of ordered quantity shall undergo external pressure testing at 5,000 psi.
In order meet F2 requirement, our manufacturer carried out this test on 3 No’s (5%) of Mandrels and one of the mandrels was found to be collapsed at 4,000 psi during the test and consequently, this mandrel was scrapped.
Vendor carried out the root cause investigation and found that yield strength for raw material (API 5CT L-80, 80,000 psi yield strength grade) is found to be less than the minimum.
i.e. 72 ksi (tested & measured value) below the minimum required limit 80 ksi (API 5CT).
After this, remaining all 24 Mandrels were re-heat treated to achieve 80 ksi yield strength and subsequently, again 3 No’s (5%) of Mandrels were externally pressure tested at 5,000 psi and successfully passed.
My questions are :
1)Can we ask vendor to perform 100% external pressure test on all 24 No’s as a penalty & to ensure integrity of all mandrels?
OR 5% ( 3No’s) would be suffice to assure the integrity of remaining quantity ?? It has to be noted that API 19G1 does not call for any penalty in case of failure if any of external pressure testing.
2)Does yield strength under value (below 80 ksi) really attribute to external pressure testing failure (collapse) ?
3)What are factors to be considered to mitigate such failures in future ?
Regards
We have ordered Side Pocket Mandrels (Quantity: 50 No’s) with monogram & testing to API 1G1 V1 F2.
As per API 19G1, for F2 grade, 5% of ordered quantity shall undergo external pressure testing at 5,000 psi.
In order meet F2 requirement, our manufacturer carried out this test on 3 No’s (5%) of Mandrels and one of the mandrels was found to be collapsed at 4,000 psi during the test and consequently, this mandrel was scrapped.
Vendor carried out the root cause investigation and found that yield strength for raw material (API 5CT L-80, 80,000 psi yield strength grade) is found to be less than the minimum.
i.e. 72 ksi (tested & measured value) below the minimum required limit 80 ksi (API 5CT).
After this, remaining all 24 Mandrels were re-heat treated to achieve 80 ksi yield strength and subsequently, again 3 No’s (5%) of Mandrels were externally pressure tested at 5,000 psi and successfully passed.
My questions are :
1)Can we ask vendor to perform 100% external pressure test on all 24 No’s as a penalty & to ensure integrity of all mandrels?
OR 5% ( 3No’s) would be suffice to assure the integrity of remaining quantity ?? It has to be noted that API 19G1 does not call for any penalty in case of failure if any of external pressure testing.
2)Does yield strength under value (below 80 ksi) really attribute to external pressure testing failure (collapse) ?
3)What are factors to be considered to mitigate such failures in future ?
Regards