Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations cowski on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

What type of plating to use? 2

Status
Not open for further replies.

jackpot

Materials
Apr 27, 2004
25
If a steel spring (1080) comes in contact with 2024 aluminum will galvanic corrosion initiate (clean environment)? Would a zinc plating help minimize the risk.

Thanks Jack
 
Replies continue below

Recommended for you

Galvanic corrosion can occur if the two metals are in contact and an electrolyte is present. Mechanical zinc plating (not electroplating, due to the high hardness of the spring steel and the resulting embrittlement) would be one solution. An organic coating such as those supplied by Magni, D[ö]rken, or Metal Coatings would be better.

Regards,

Cory

Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 
yes and yes. of course 1080 in the Q&T condition is quite rust prone. and zinc coatings really tend to not be the most sucessfull way to protect parts in this environment. i would use a plastic to completely isolate the two materials. you need to prevent conductive contact between steels and aluminium.
 
This assembly is used in an aerospace application.
 