Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations cowski on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Welding to galvanized steel

Status
Not open for further replies.

LKK

Structural
Jan 14, 2002
3
How galvanization is going to be affected by welding. I am aware that galvanization needs to be removed before welding, and then it can be restored - what is the lifetime of restored area? Has anybody have any experience with welding Nelson studs to galvanized beams?
 
Replies continue below

Recommended for you

Here is an example, tested by bending.
Typically the explosive nature of stud welding removes enough zinc to produce a good weld. Increase the weld time and/or amperage may be required.
91250010.jpg


If you have to make a repair use SMAW and 6010 electrode. (The rutile flusx improves the weld.)
 
LKK -- The American Galvanizers Association ("AGA") has two publications that you'd find useful: Welding & Hot-Dip Galvanizing, and the Inspection of Products Hot-Dip Galvanized After Fabrication, Including A New Section on Touch-up & Repair. You may request complimentary copies from the AGA, 800-468-7732, or you may download them from the AGA Web site, We're also available to answer any other questions you may have regarding hot-dip galvanizing after fabrication (not galvanized sheet/strip products).
 