HELLO

I WANT TO KNOW WHICH FILLER WIRE SHALL BE MOST SUITABLE FOR WELDING B/W...20Cr32Ni (conc reducer) & SB-407 N 8810 (pipe) .

SOME POSSIBLE MAY BE:

INCONEL 82
INCONEL 625
INCONEL 617

THANKING U PPL IN ADVANCE.
 
Replies continue below

Recommended for you

Any of those would make a sound weld. Typically 82 bare wire or 182 electrode is used to weld 800H to itself.

The type 617 wires or 117 electrodes are used if high creep strength is desirable in the weld. 82/182 welds will be weaker at temperature than the 800H base metal, but have excellent ductility.
 