Any of those would make a sound weld. Typically 82 bare wire or 182 electrode is used to weld 800H to itself.
The type 617 wires or 117 electrodes are used if high creep strength is desirable in the weld. 82/182 welds will be weaker at temperature than the 800H base metal, but have excellent ductility.