Mar 16, 2021 #1 jagadeesh310 Mechanical Joined Mar 16, 2021 Messages 1 Location IN For IS2062 GR.B plate to plate welding can i use E8012-b2 welding electrode
Mar 16, 2021 #2 DVWE Petroleum Joined Apr 5, 2007 Messages 2,368 Location US Yes, it can be done. There is a little extra chromium (~1.25%) and tensile over match with a B2 electrode, but it all depends on the application for which the plate is used. The devil is in the details; she also wears prada. Upvote 0 Downvote
Yes, it can be done. There is a little extra chromium (~1.25%) and tensile over match with a B2 electrode, but it all depends on the application for which the plate is used. The devil is in the details; she also wears prada.
Mar 18, 2021 #3 weldstan Materials Joined Jun 24, 2011 Messages 2,806 Location US Because this is not a low hydrogen electrode preheating will be required to mitigate potential for hydrogen induced cracking. Upvote 0 Downvote
Because this is not a low hydrogen electrode preheating will be required to mitigate potential for hydrogen induced cracking.
Mar 19, 2021 #4 Guest Is that all you need to know about welding Cr-Mo steel? "Everyone is entitled to their own opinions, but they are not entitled to their own facts." Upvote 0 Downvote
Is that all you need to know about welding Cr-Mo steel? "Everyone is entitled to their own opinions, but they are not entitled to their own facts."
Mar 19, 2021 #5 weldstan Materials Joined Jun 24, 2011 Messages 2,806 Location US The steel grade to be welded is a low carbon steel. There are certainly better alternative electrodes for the purpose. Upvote 0 Downvote
The steel grade to be welded is a low carbon steel. There are certainly better alternative electrodes for the purpose.
Mar 19, 2021 #6 dik Structural Joined Apr 13, 2001 Messages 26,115 Location CA I like low hydrogen, myself... Rather than think climate change and the corona virus as science, think of it as the wrath of God. Feel any better? -Dik Upvote 0 Downvote
I like low hydrogen, myself... Rather than think climate change and the corona virus as science, think of it as the wrath of God. Feel any better? -Dik