Dear All
I need your help for this matter.
I have to weld A335-P11 (1-1/4 Cr - ½ Mo) to A106B (Carbone Steel).
Construction Code ASME B31.3 (Process Piping)
I have a qualified PQR
Base Metal: A335-P11 to A335-P11 P4.1 as per ASME IX – QW-422
Process welding: SMAW
Filler Metal: E8018-B2 F No 4 A No 3
I Will use a WPS (P4.1 to P1.1) according to ASME IX – QW-424.1
Base Metal(s) Used for Procedure Qualification Coupon:
One metal from P‐No. 4 to any metal from P‐No. 4
Base Metals Qualified:
Any P‐No. 4 metal to any metal assigned P‐No. 4, 3, or 1
My question: Can I use E8018-B2 electrode to weld these dissimilar base metals while AWS D10.8 Table 2 suggest to use E7018 to weld 1-1/4 Cr-0.5Mo (A335-P11) to C-Steel (A106-B).
In the same code
Para. 3.4.2 Joining dissimilar Ferritic Steels. Where dissimilar metals are being welded, the only four possible filler metal composition are:
1. The lower alloy base metal composition,
2. the higher alloy base metal composition,
3. an intermediate composition, or
4. a composition different from any of the first three.
Where both base metals are ferritic , the fourth possibility mentioned above (that of an entirely different alloy) is of special concern for service at elevated temperatures or in corrosive environments. Consistent with the factors listed above, this fourth possibility should normally be considered only where one of the base metals is stainless steel or nickel or copper alloy.
and an other code
API RP 5826.2 Dissimilar Welding
6.2.1 When joining dissimilar ferritic steels (P-1 though P-5), the filler metal shall conform to the nominal chemical composition of either base metal or an intermediate composition. However, when attaching nonpressure parts to pressure parts the filler metal chemical composition shall match the nominal chemical composition of the pressure part.
Below some extracts from ASME II Part. A & C
E8018-B2C
Mn Si P S Ni Cr Mo
0.05–0.12 0.90 0.80 0.03 0.03 . . . 1.00–1.50 0.40–0.65
A 335-P11C
Mn Si P S Ni Cr Mo
0.05–0.15 0.30–0.60 0.50–1.00 0.025 0.025 … 1.00–1.50 0.44–0.65
---------------------------------------------------------------------------------------------------------------------------------------------
E7018C
Mn Si P S Ni Cr Mo V Mn + Ni + Cr + Mo + V
0.15 1.60 0.75 0.035 0.035 0.30 0.20 0.30 0.08 1.75
A106-BC
Mn Si P S Ni Cr Mo V Mn + Ni + Cr + Mo + V
0.30 0.29–1.06 0.10 0.035 0.035 0.40 0.40 0.15 0.08
--------------------------------------------------------------------------------------------------------------------------------------------------
Thanks in advance
And Best wishes from Algeria
I need your help for this matter.
I have to weld A335-P11 (1-1/4 Cr - ½ Mo) to A106B (Carbone Steel).
Construction Code ASME B31.3 (Process Piping)
I have a qualified PQR
Base Metal: A335-P11 to A335-P11 P4.1 as per ASME IX – QW-422
Process welding: SMAW
Filler Metal: E8018-B2 F No 4 A No 3
I Will use a WPS (P4.1 to P1.1) according to ASME IX – QW-424.1
Base Metal(s) Used for Procedure Qualification Coupon:
One metal from P‐No. 4 to any metal from P‐No. 4
Base Metals Qualified:
Any P‐No. 4 metal to any metal assigned P‐No. 4, 3, or 1
My question: Can I use E8018-B2 electrode to weld these dissimilar base metals while AWS D10.8 Table 2 suggest to use E7018 to weld 1-1/4 Cr-0.5Mo (A335-P11) to C-Steel (A106-B).
In the same code
Para. 3.4.2 Joining dissimilar Ferritic Steels. Where dissimilar metals are being welded, the only four possible filler metal composition are:
1. The lower alloy base metal composition,
2. the higher alloy base metal composition,
3. an intermediate composition, or
4. a composition different from any of the first three.
Where both base metals are ferritic , the fourth possibility mentioned above (that of an entirely different alloy) is of special concern for service at elevated temperatures or in corrosive environments. Consistent with the factors listed above, this fourth possibility should normally be considered only where one of the base metals is stainless steel or nickel or copper alloy.
and an other code
API RP 5826.2 Dissimilar Welding
6.2.1 When joining dissimilar ferritic steels (P-1 though P-5), the filler metal shall conform to the nominal chemical composition of either base metal or an intermediate composition. However, when attaching nonpressure parts to pressure parts the filler metal chemical composition shall match the nominal chemical composition of the pressure part.
Below some extracts from ASME II Part. A & C
E8018-B2C
Mn Si P S Ni Cr Mo
0.05–0.12 0.90 0.80 0.03 0.03 . . . 1.00–1.50 0.40–0.65
A 335-P11C
Mn Si P S Ni Cr Mo
0.05–0.15 0.30–0.60 0.50–1.00 0.025 0.025 … 1.00–1.50 0.44–0.65
---------------------------------------------------------------------------------------------------------------------------------------------
E7018C
Mn Si P S Ni Cr Mo V Mn + Ni + Cr + Mo + V
0.15 1.60 0.75 0.035 0.035 0.30 0.20 0.30 0.08 1.75
A106-BC
Mn Si P S Ni Cr Mo V Mn + Ni + Cr + Mo + V
0.30 0.29–1.06 0.10 0.035 0.035 0.40 0.40 0.15 0.08
--------------------------------------------------------------------------------------------------------------------------------------------------
Thanks in advance
And Best wishes from Algeria