hello,

I need info about welding (corner weld 2 passes) st 37 on a 4140 shaft. Can this be welded with 16%Cr and 65 % Ni electrode ?
 
Don't know what st37 is, but you should give a lot of consideration to the HAZ of the 4140, which will probably be quite hard and brittle if you don't use enough preheat. Post weld HT is better.
 
Are you referring to ENiCrFe2 type of electrode? I.e. Inco-Weld A from |Special Metals for e.g. Refer this link for details Yes, this consumable can be used for the application detailed. Refer to Metalguy's words of caution though.
Metalguy
for St37 refer following posts:
thread330-62886 refersa to St37 which is equivalent of S235
thread330-56039 refers to USt37-2 which is equivalent of A283
Finally see the last post in thread330-17608 which explains what St37 stands for!!!

Thanks and regards
Sayee Prasad R
Ph: 0097143968906
Mob: 00971507682668
email: sayee_prasad@yahoo.com
The whole of science is nothing more than a refinement of everyday thinking!!! [thumbsup]
 
Metalguy,

Thanks for reply
Shaft will be preheated at 250degree C(482 degree F) . After welding, the shaft will be "insulated" during some time, so cooling will be slowly.

St 37 Analyse : %C <=0.17
%Si <= 0.55
%Mn <=1.60
%P <=0.04
%S <=0.04
 
Your intended preheat is pretty good, but I'd go even higher. What you want to do is avoid cooling thru the range of ~1,300 to 1,000 deg F too fast. This will allow time for the austenite in the HAZ to transform to pearlite.

I did a little study with a low alloy steel (P3) welded with the worst case-a single pass. Preheating to 400 deg. F. wasn't high enough, but we never did go back and try higher temps.
 
JimMetalsCeramics,

This is a proposal from manufacturer
 
If your stuck with it, I would use a high preheat and a slow-cool down. But it's too Cr-rich for my tastes.

 